Tensile test of 1.4541 / X6CrNi18-10 / AISI 321 grade austenitic steel
Open Research DataShip structures and their components are build mainly of steel. Hull steel is used to build the hull structure. Some structural elements, such as RSW (Refrigerated See Water) tanks, or LNG (Liquid Natural Gas) tanks - gas transported at temperatures below -162° C, are build from austenitic steels. Austenitic steels have a different microstructure and...
-
Tensile test of 1.4571 / X6CrNiMoTi17-12-2 / AISI 316Ti grade austenitic steel
Open Research DataShip structures and their components are build mainly of steel. Hull steel is used to build the hull structure. Some structural elements, such as RSW (Refrigerated See Water) tanks, or LNG (Liquid Natural Gas) tanks - gas transported at temperatures below -162° C, are build from austenitic steels. Austenitic steels have a different microstructure and...
-
STL files of all-3D-printable electrochemical cell
Open Research DataThis dataset contains STL files required for fabrication of an all 3D printed electrochemical cell, that can be used in electroanalytical studies.
-
The AFM micrographs of pitting corrosion evolution on high-alloy steel 1.4301
Open Research DataThe dataset contains the results of topographic imaging of high-alloy stainless steel 1.4301 on which the pitting corrosion process was induced by electrochemical methods. The study of the effects of a local attack allows for conclusions about the intensity and mechanism of this type of corrosion. The file contains atomic force microscopy (AFM) data...
-
Determination of mechanical properties of Ti13Nb13Zr cubes made with STL technology subjected to uniaxial compression
Open Research DataThe aim of the study was to determine the mechanical properties of Ti13Nb13Zr cubes made with STL technology (3D printing). The experiments were carried out on the Hung Ta universal test machine HT-2402. Cubes with the initial dimensions of 10x10x10 mm were subjected to compression by increasing force to over 80 kN. In various experiments, the angle...
-
X-ray diffraction (XRD) of pristine bismuth oxide (Bi2O3) and gadolinium oxide (Gd2O3) structures
Open Research DataData contain results from X-ray diffraction (XRD) measurements of pristine Bi2O3 and Gd2O3 structures using Aeris diffractometer (Malvern Panalytical, Malvern, UK) with Cu-Kα radiation (λ = 1.544 Å)
-
Measurement file of PEEK 70 mm bushing measurements in original condition perforemed on custom-built 3d measuring stand
Open Research DataAfter manufacturing process (lathe turning) bearing was measured on custom bulit measurement stan developed during research project financed by National Centre of Science. Measurements consist of 110 000 points in 3D space taken on bushing inner surface. Bearing was measured taking vertical steps of 0,2 mm.
-
Phoenix 3D models
Open Research DataThe dataset includes the generated raw, unstructured triangulated surface files, under STL format, employed as geometries for the Computational Fluid Dynamics (CFD) simulations, as part of the 2022/45/B/ST8/02847 NCN OPUS Project
-
X-ray diffraction patterns of BaCe0.6Zr0.2Y0.2-xFexO3-δ (x = 0.02, 0.05, 0.1)
Open Research DataThe dataset consists of three raw X-ray diffraction (XRD) files collected using a Phillips X’Pert Pro diffractometer (CuKα radiation (𝜆 = 1.541 Å), under 40 kV and 30 mA). The diffraction patterns of BaCe0.6Zr0.2Y0.18Fe0.02O3-δ (BCZYFe2), BaCe0.6Zr0.2Y0.15Fe0.05O3-δ (BCZYFe5), and BaCe0.6Zr0.2Y0.1Fe0.1O3-δ (BCZYFe10) were collected at room temperature....
-
SiC coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #B37/#A35
Open Research DataWear tests in sliding friction of SiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, SiC over SiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 3 min.Secimen...
-
TiC coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #A39/#B41
Open Research DataWear tests in sliding friction of TiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiC over TiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 3 min.Secimen...
-
SiC coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #A35/#B37
Open Research DataWear tests in sliding friction of SiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, SiC over SiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 3 min.Secimen...
-
Data used for article "Chemical composition and techno-functional properties of high-purity water-soluble keratein and its enzymatic hydrolysates"
Open Research DataThe dataset contains data regarding chicken feather keratin isolate (KI) obtained by reductive extraction with L-cysteine and its enzymatic hydrolysates produced by trypsin (KI-T), chymotrypsin (KI-C), pepsin (KI-P) and subtilisin (KI-S). The dataset includes data on the keratin extraction yield (% of feather solubilization), data from high-performance...
-
X-ray diffraction (XRD) of silica-coated bismuth oxide (Bi2O3) and gadolinium oxide (Gd2O3) structures
Open Research DataData contain results from X-ray diffraction (XRD) measurements of pristine Bi2O3 and Gd2O3 structures using Aeris diffractometer (Malvern Panalytical, Malvern, UK) with Cu-Kα radiation (λ = 1.544 Å)
-
X-ray diffraction (XRD) of silica-coated bismuth oxide/gadolinium oxide (Bi2O3+Gd2O3) structures
Open Research DataData contain results from X-ray diffraction (XRD) measurements of pristine Bi2O3 and Gd2O3 structures using Aeris diffractometer (Malvern Panalytical, Malvern, UK) with Cu-Kα radiation (λ = 1.544 Å)
-
Thermal stability of V2O5 nanorods under oxidizing atmosphere
Open Research DataThe DataSet contains the TGA curves of V2O5 nanorods obtained at 650°C. The information about nanorods synthesis is described in the Journal of Nanomaterials.
-
Changes in heat flow of V2O5 nanorods under oxidizing atmosphere
Open Research DataThe DataSet contains the DSC curves of V2O5 nanorods obtained at 650°C. The information about nanorods synthesis is described in the Journal of Nanomaterials.
-
The XRD diffraction patterns of Ce(Pr,Sm)O2-s samples
Open Research DataThe dataset includes XRD diffraction patterns of Ce(Pr,Sm)O2-s samples of various stoichiometries of Pr and Sm dopants. Samples were produced using aqueous soft chemistry methods (microemulsion method).
-
Decomposition kinetics of vanadium xerogel powder
Open Research DataThe DataSet contains the TGA curves of vanadium As-prepared xerogel powder with different heating rates. The information about sol synthesis is described in the Journal of Nanomaterials.
-
CrN coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #A23/#B22
Open Research DataWear tests in sliding friction of CrN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, CrN over CrN . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 12 min. The...
-
CrN coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #A25/#B21
Open Research DataWear tests in sliding friction of CrN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, CrN over CrN . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 9 min....
-
TiN coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #B48/#A45
Open Research DataWear tests in sliding friction of TiN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiN over TiN . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 12 min....
-
SiC coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #B34/#A33
Open Research DataWear tests in sliding friction of SiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, SiC over SiC. Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 3 min. The test...
-
TiN coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #A45/#B48
Open Research DataWear tests in sliding friction of TiN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiN over TiN . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 12 min....
-
TiC coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #B41/#A39
Open Research DataWear tests in sliding friction of TiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiC over TiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 9 min....
-
TiC coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #A41/#B39
Open Research DataWear tests in sliding friction of TiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiC over TiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 3 min. The...
-
CrN coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #B22/#A23
Open Research DataWear tests in sliding friction of CrN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, CrN over CrN. Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 6 min. The test...
-
SiC coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #A33/#B34
Open Research DataWear tests in sliding friction of SiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, SiC over SiC. Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 3 min. The test...
-
TiC coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #B39/#A41
Open Research DataWear tests in sliding friction of TiC coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiC over TiC . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 3 min. The test...
-
Thermal stability of V2O5 nanorods under inert atmosphere
Open Research DataThe DataSet contains the TGA curves of V2O5 nanorods obtained at 650°C. The information about nanorods synthesis is described in the Journal of Nanomaterials.
-
Thermal behaviour of vanadium xerogel powder under different inert atmosphere
Open Research DataThe DataSet contains the results of the thermal behavior of the vanadium xerogel powder. The information about xerogel powder synthesis is described in the Journal of Nanomaterials.
-
Crystallization kinetics of V2O5 nanorods
Open Research DataThe DataSet contains the DSC curves of As-prepared xerogel powder with different heating rates. The information about sol synthesis is described in the Journal of Nanomaterials.
-
Thermal stability of vanadium xerogel powder under different atmpshere
Open Research DataThe DataSet contains the results of the thermal behavior of the vanadium xerogel powder. The information about xerogel powder synthesis is described in the Journal of Nanomaterials.
-
Changes in heat flow of V2O5 nanorods under inert atmosphere
Open Research DataThe DataSet contains the DSC curves of V2O5 nanorods obtained at 650°C. The information about nanorods synthesis is described in the Journal of Nanomaterials.
-
TiN coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #A45/#A47
Open Research DataWear tests in sliding friction of TiN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiN over TiN. Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 20 min. The test...
-
CrN coating in ring-on-ring sliding with saline solution (0.9%) lubrication 5MPa, 0.1m/s specimn. #B21/#A21
Open Research DataWear tests in sliding friction of CrN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, CrN over CrN . Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: SALINE SOLUTION (0.9%). Tribometer: PT-3. Overall test time till coating penetration 25 min....
-
TiN coating in ring-on-ring sliding with distlled water lubrication 5MPa, 0.1m/s specimn. #A45/#B45
Open Research DataWear tests in sliding friction of TiN coating on 1.4021 (EN 10088-1) heat treated stainless steel. Ring - on - ring contact in unidirectional sliding, TiN over TiN. Mean contact stress: 5MPa. Sliding velocity: 0,1 m/s. Mean friction radius: 9.5mm. Lubricant: DISTILLED WATER. Tribometer: PT-3. Overall test time till coating penetration 90 min. The test...
-
X-ray diffraction patterns of BaCe0.6Zr0.2Y0.1M0.1O3-δ (M = Fe, Pr, Tb)
Open Research DataThe dataset consists of three raw X-ray diffraction (XRD) files collected using a Phillips X’Pert Pro diffractometer (CuKα radiation (𝜆 = 1.541 Å), under 40 kV and 30 mA). The diffraction patterns of BaCe0.6Zr0.2Y0.1Fe0.1O3-δ (BCZYFe), BaCe0.6Zr0.2Y0.1Pr0.1O3-δ (BCZYPr), and BaCe0.6Zr0.2Y0.1Tb0.1O3-δ (BCZYTb) were collected at room temperature. Collected...
-
Changes in heat of vanadium xerogel powder under different atmosphere
Open Research DataThe DataSet contains the DSC curves of the vanadium xerogel powder. The information about xerogel powder synthesis is described in the Journal of Nanomaterials.
-
DSC measurments of ammonium vanadate nanocrystals
Open Research DataThe DataSet contains the thermal behavior of the ammonium vanadate nanostructures obtained by the hydrothermal method with different conditions. Differential scanning calorimetry (DSC) measurement was carried out under an argon atmosphere from 40C to 560C (with a heating rate of 10 C/min) using Netzsch STA 449 F1. The results reveal the differences...
-
Thermal behaviour of vanadium xerogel powder and V2O5 nanorods under helium atmosphere
Open Research DataThe DataSet contains the results of the thermal behavior of the vanadium xerogel powder and V2O5 nanorods obtained at 650C. The information about xerogel powder and V2O5 nanorods synthesis is described in the Journal of Nanomaterials.
-
Thermal properties of VO2 and V2O3 nanostructures
Open Research DataThe DataSet contains the DSC and TG curves of VO2 and V2O3 nanostructures obtained by the sol-gel with different reaction conditions. The information about xerogel powder synthesis is described in the Journal of Nanomaterials. The xerogel powder was annealing under argon atmosphere at the selected temperature: 500C, 600C, and 1000C.
-
Morphological and electrochemical characterization of ceramic carbon foam electrodes water treatment applications
Open Research DataThis dataset contains morphological and electrochemical characterization of ceramic carbon foam employed as an electrode (CFFE) for the oxidation of a target pollutant. The dataset includes:
-
Miscanthus × giganteus growth and photosynthetic rate measurements
Open Research DataThis data set contains the findings of the growth development, gas exchange, and specific leaf area of the plants during the experiment in which straw and wood chips-based biochars were used as soil amendment for Miscanthus × giganteus (M×g) cultivation.
-
Electrocatalytic water splitting by bifunctional Zircon-doped borophene
Open Research DataThe data in the folder represent modified boron for use in electrochemical water splitting half reactions. The oxygen evolution reaction (OER) and hydrogen evolution reaction (HER) play a vital role in renewable energy applications such as water splitting. Borophene, a two-dimensional (2D) boron-based material, has garnered significant attention due...
-
DSC and TG results for strontium ferrite molybdate: pristine La, or Nb-doped
Open Research DataThis dataset consists of DSC and TG data collected for SFM, LSFM (La-doped) and SFMNb (Nb-doped) compounds, which were undertaken to analyze the reoxidation process of reduced compounds and its transition to double-perovskite structure .The appropriate amount of the powder (~10 mg with 10% tolerance factor) were placed into the alumina crucible and...
-
Thermal behavior of (NH4)V4O10xH2O
Open Research DataThe DataSet contains the results of the thermal behavior of the (NH4)V4O10xH2O obtained by the hydrothermal method using different precursors: microstructured (commercially available) or nanostructured. The information about samples synthesis is described in the Materials.
-
Thermal behaviour of vanadium xerogel powder under oxidizing atmosphere
Open Research DataThe DataSet contains the results of the thermal behavior of the vanadium xerogel powder. The information about xerogel powder synthesis is described in the Journal of Nanomaterials.
-
Thermal behaviour of vanadium xerogel powder under argon atmosphere
Open Research DataThe DataSet contains the results of the thermal behavior of the vanadium xerogel powder. The information about xerogel powder synthesis is described in the Journal of Nanomaterials.
-
Number of statements issued about the intention to entrust the performance of work and the dynamics of change (%, year to year) in 2008-2018
Open Research DataWhen analyzing data on declarations of intention to entrust work to a foreigner, whose registration was completed at the end of 2017, with data on declarations on entrusting work to a foreigner, effective from 01/01/2018, it should noted that since 2018 the scope of data regarding statements. Currently they apply only to works that are not considered...